{"id":52064,"date":"2024-09-30T08:10:10","date_gmt":"2024-09-30T06:10:10","guid":{"rendered":"https:\/\/welding-alloys.zerobox.co.za\/?p=52064"},"modified":"2024-09-30T15:20:35","modified_gmt":"2024-09-30T13:20:35","slug":"comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue","status":"publish","type":"post","link":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/","title":{"rendered":"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue"},"content":{"rendered":"<div id='full_slider_1'  class='avia-fullwidth-slider main_color avia-shadow   avia-builder-el-0  el_before_av_section  avia-builder-el-first   container_wrap sidebar_left'  >\n<style type=\"text\/css\" data-created_by=\"avia_inline_auto\" id=\"style-css-av-m1hwa29l-fb2ad8657a08be4c0579e0360e99aafc\">\n#top #wrap_all .avia-slideshow .av-slideshow-caption.av-m1hwa29l-fb2ad8657a08be4c0579e0360e99aafc__0 .avia-caption-title{\nfont-size:38px;\ncolor:#ffffff;\n}\n<\/style>\n<div  class='avia-slideshow av-m1hwa29l-fb2ad8657a08be4c0579e0360e99aafc avia-slideshow-no scaling av_slideshow_full avia-slide-slider av-slideshow-ui av-control-default av-slideshow-manual av-loop-once av-loop-manual-endless av-default-height-applied   avia-slideshow-1' data-slideshow-options=\"{&quot;animation&quot;:&quot;slide&quot;,&quot;autoplay&quot;:false,&quot;loop_autoplay&quot;:&quot;once&quot;,&quot;interval&quot;:5,&quot;loop_manual&quot;:&quot;manual-endless&quot;,&quot;autoplay_stopper&quot;:false,&quot;noNavigation&quot;:false,&quot;bg_slider&quot;:false,&quot;keep_padding&quot;:false,&quot;hoverpause&quot;:false,&quot;show_slide_delay&quot;:0}\"  itemprop=\"image\" itemscope=\"itemscope\" itemtype=\"https:\/\/schema.org\/ImageObject\" ><ul class='avia-slideshow-inner ' style='padding-bottom: 24.609375%;'><li  class='avia-slideshow-slide av-m1hwa29l-fb2ad8657a08be4c0579e0360e99aafc__0  av-single-slide slide-1 slide-odd'><div data-rel='slideshow-1' class='avia-slide-wrap '   ><div class='av-slideshow-caption av-m1hwa29l-fb2ad8657a08be4c0579e0360e99aafc__0 caption_fullwidth caption_left caption_left_framed caption_framed'><div class=\"container caption_container\"><div class=\"slideshow_caption\"><div class=\"slideshow_inner_caption\"><div class=\"slideshow_align_caption\"><h2 class='avia-caption-title '  itemprop=\"name\" >Quoi de neuf chez Welding Alloys ?<\/h2><\/div><\/div><\/div><\/div><\/div><img decoding=\"async\" fetchpriority=\"high\" class=\"wp-image-10044 avia-img-lazy-loading-not-10044\"  src=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/01\/news-banner.jpg\" width=\"1280\" height=\"315\" title='news banner' alt='news banner'  itemprop=\"thumbnailUrl\"  style='min-height:250px; min-width:1016px; ' srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/01\/news-banner.jpg 1280w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/01\/news-banner-600x148.jpg 600w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/01\/news-banner-300x74.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/01\/news-banner-500x123.jpg 500w\" sizes=\"(max-width: 1280px) 100vw, 1280px\" \/><\/div><\/li><\/ul><\/div><\/div>\n<div id='av_section_1'  class='avia-section av-av_section-b18f66ddd9f3a20c8cf3795743e7d7ea alternate_color avia-section-small avia-no-border-styling  avia-builder-el-1  el_after_av_slideshow_full  el_before_av_section  breadcrumb-container avia-bg-style-scroll container_wrap sidebar_left'  ><div class='container av-section-cont-open' ><div class='template-page content  av-content-small units'><div class='post-entry post-entry-type-page post-entry-52064'><div class='entry-content-wrapper clearfix'>\n\n\n<\/div><\/div><\/div><!-- close content main div --><\/div><\/div><div id='av_section_2'  class='avia-section av-av_section-2dcb3d115e2e5af9a73072e0505910f8 main_color avia-section-default avia-no-border-styling  avia-builder-el-3  el_after_av_section  el_before_av_one_full  avia-bg-style-scroll container_wrap sidebar_left'  ><div class='container av-section-cont-open' ><div class='template-page content  av-content-small units'><div class='post-entry post-entry-type-page post-entry-52064'><div class='entry-content-wrapper clearfix'>\n<div class='flex_column_table av-av_one_full-6bea7e7def1bbc5ff1eddab54a2a43d7 sc-av_one_full av-equal-height-column-flextable'><div  class='flex_column av-av_one_full-6bea7e7def1bbc5ff1eddab54a2a43d7 av_one_full  avia-builder-el-4  el_before_av_one_full  avia-builder-el-first  first no_margin flex_column_table_cell av-equal-height-column av-align-top av-animated-generic left-to-right  '     ><p>\n<style type=\"text\/css\" data-created_by=\"avia_inline_auto\" id=\"style-css-av-m1hmaxm1-6bb561632a8d4f2d4138cdd96de58625\">\n#top .av-special-heading.av-m1hmaxm1-6bb561632a8d4f2d4138cdd96de58625{\npadding-bottom:10px;\n}\nbody .av-special-heading.av-m1hmaxm1-6bb561632a8d4f2d4138cdd96de58625 .av-special-heading-tag .heading-char{\nfont-size:25px;\n}\n.av-special-heading.av-m1hmaxm1-6bb561632a8d4f2d4138cdd96de58625 .av-subheading{\nfont-size:15px;\n}\n<\/style>\n<div  class='av-special-heading av-m1hmaxm1-6bb561632a8d4f2d4138cdd96de58625 av-special-heading-h1 blockquote modern-quote  avia-builder-el-5  el_before_av_social_share  avia-builder-el-first '><h1 class='av-special-heading-tag '  itemprop=\"headline\"  >Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue<\/h1><div class='av-subheading av-subheading_below'><a href=\"https:\/\/welding-alloys.zerobox.co.za\/fr\/secteur\/siderurgie\/\">Sid\u00e9rurgie<\/a>\n<\/div><div class=\"special-heading-border\"><div class=\"special-heading-inner-border\"><\/div><\/div><\/div><br \/>\n<div  class='av-social-sharing-box av-av_social_share-34505b183a6fb217f4212e33accee550 av-social-sharing-box-icon-simple  avia-builder-el-6  el_after_av_heading  avia-builder-el-last  av-social-sharing-box-same-width'><div class=\"av-share-box\"><h5 class='av-share-link-description av-no-toc '>Partager cet article<\/h5><ul class=\"av-share-box-list noLightbox\"><li class='av-share-link av-social-link-facebook avia_social_iconfont' ><a target=\"_blank\" aria-label=\"Partager sur Facebook\" href='https:\/\/www.facebook.com\/sharer.php?u=https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/&#038;t=Comprendre%20et%20Combattre%20L%E2%80%99usure%20sur%20les%20Rouleaux%20de%20Coul%C3%A9e%20Continue' data-av_icon='\ue8f3' data-av_iconfont='entypo-fontello'  title='' data-avia-related-tooltip='Partager sur Facebook'><span class='avia_hidden_link_text'>Partager sur Facebook<\/span><\/a><\/li><li class='av-share-link av-social-link-linkedin avia_social_iconfont' ><a target=\"_blank\" aria-label=\"Partager sur LinkedIn\" href='https:\/\/linkedin.com\/shareArticle?mini=true&#038;title=Comprendre%20et%20Combattre%20L%E2%80%99usure%20sur%20les%20Rouleaux%20de%20Coul%C3%A9e%20Continue&#038;url=https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/' data-av_icon='\ue8fc' data-av_iconfont='entypo-fontello'  title='' data-avia-related-tooltip='Partager sur LinkedIn'><span class='avia_hidden_link_text'>Partager sur LinkedIn<\/span><\/a><\/li><li class='av-share-link av-social-link-mail avia_social_iconfont' ><a  aria-label=\"Partager par Mail\" href='mailto:?subject=Comprendre%20et%20Combattre%20L%E2%80%99usure%20sur%20les%20Rouleaux%20de%20Coul%C3%A9e%20Continue&#038;body=https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/' data-av_icon='\ue805' data-av_iconfont='entypo-fontello'  title='' data-avia-related-tooltip='Partager par Mail'><span class='avia_hidden_link_text'>Partager par Mail<\/span><\/a><\/li><\/ul><\/div><\/div><\/p><\/div><\/div><!--close column table wrapper. Autoclose: 1 --><div class='flex_column_table av-av_one_full-876c75c95304012b3250e44391fb5c8f sc-av_one_full av-equal-height-column-flextable'>\n<style type=\"text\/css\" data-created_by=\"avia_inline_auto\" id=\"style-css-av-av_one_full-876c75c95304012b3250e44391fb5c8f\">\n#top .flex_column_table.av-equal-height-column-flextable.av-av_one_full-876c75c95304012b3250e44391fb5c8f{\nmargin-top:15px;\nmargin-bottom:0px;\n}\n<\/style>\n<div  class='flex_column av-av_one_full-876c75c95304012b3250e44391fb5c8f av_one_full  avia-builder-el-7  el_after_av_one_full  el_before_av_one_full  first no_margin flex_column_table_cell av-equal-height-column av-align-top av-animated-generic left-to-right  column-top-margin'     ><section  class='av_textblock_section av-m1hmetad-b40658902cd1ebeddf0274ccabc28913 '   itemscope=\"itemscope\" itemtype=\"https:\/\/schema.org\/BlogPosting\" itemprop=\"blogPost\" ><div class='avia_textblock'  itemprop=\"text\" ><p>La coul\u00e9e continue joue un r\u00f4le essentiel dans l&#8217;industrie sid\u00e9rurgique, en transformant l&#8217;acier en fusion en brames, billettes ou blooms. L&#8217;efficacit\u00e9 et la durabilit\u00e9 des rouleaux de coul\u00e9e continue sont ainsi cruciales pour ce processus, car ils doivent r\u00e9sister \u00e0 des conditions difficiles et \u00e0 diverses formes d&#8217;usure pendant leur fonctionnement.<\/p>\n<p>Opter pour les fils fourr\u00e9s de Welding Alloys pour prot\u00e9ger les rouleaux garantit un rechargement de haute qualit\u00e9, en r\u00e9duisant consid\u00e9rablement les co\u00fbts de maintenance et les arr\u00eats de production, conduisant \u00e0 des \u00e9conomies \u00e0 long terme. Welding Alloys propose des solutions de rechargement pour les rouleaux neufs et usag\u00e9s, garantissant des performances optimales et une rentabilit\u00e9 accrue.<\/p>\n<p><strong>CORRESIST \u2192 Am\u00e9liorez les performances des segments sup\u00e9rieur<\/strong><strong>s de vos coul\u00e9es continues<\/strong><\/p>\n<p><a href=\"https:\/\/welding-alloys.zerobox.co.za\/fr\/produit\/corresist-o\/\">CORRESIST <\/a>est un fil fourr\u00e9 qui produit un d\u00e9p\u00f4t de soudure unique en acier inoxydable super aust\u00e9nitique. Ce mat\u00e9riau est hautement r\u00e9sistant \u00e0 l&#8217;oxydation et \u00e0 la corrosion, m\u00eame dans des environnements \u00e0 haute temp\u00e9rature, ce qui le rend id\u00e9al pour le rechargement des rouleaux de la partie sup\u00e9rieure de la ligne de coul\u00e9e continue, avec les rouleaux en sortie de la lingoti\u00e8re et dans la zone cintrage (foot and bender rolls).<\/p>\n<p>La zone sup\u00e9rieure des coul\u00e9es continues subissent les temp\u00e9ratures les plus \u00e9lev\u00e9es et les conditions corrosives les plus extr\u00eames. Les rouleaux en acier inoxydable martensitique traditionnels et les mat\u00e9riaux de rechargement deviennent souvent instables dans de tels environnements, entra\u00eenant une d\u00e9t\u00e9rioration rapide. CORRESIST, gr\u00e2ce \u00e0 son alliage unique, garantit la stabilit\u00e9 et la r\u00e9sistance \u00e0 la corrosion n\u00e9cessaire, m\u00eame lorsqu&#8217;il est expos\u00e9 \u00e0 des temp\u00e9ratures extr\u00eames.<\/p>\n<p><strong>Performance:<\/strong><\/p>\n<p>CORRESIST a montr\u00e9 des am\u00e9liorations remarquables en termes de dur\u00e9e de vie et de performances des rouleaux. Par exemple, pour les rouleaux positionn\u00e9s directement sous la lingoti\u00e8re, le rechargement avec CORRESIST a permis de r\u00e9aliser :<\/p>\n<ul>\n<li><strong>650 coul\u00e9es de 110 tonnes par coul\u00e9e :<\/strong> Cette performance d\u00e9passe de mani\u00e8re significative celle des rechargements martensitiques conventionnels, qui souffrent souvent de corrosion et d&#8217;oxydation s\u00e9v\u00e8res apr\u00e8s une utilisation similaire.<\/li>\n<li><strong>Trois fois la dur\u00e9e de vie des rouleaux forg\u00e9s 17-4PH :<\/strong> Apr\u00e8s 650 coul\u00e9es, les rouleaux CORRESIST pr\u00e9sentaient moins de 0,7 mm d&#8217;usure, rendant le resurfa\u00e7age possible.<\/li>\n<\/ul>\n<p><strong>CHROMECORE \u2192 La r\u00e9ponse ultime pour les <\/strong><strong>segments interm\u00e9diaires et inf\u00e9rieurs de vos coul\u00e9es continues<\/strong><\/p>\n<p>Pour lutter efficacement contre l&#8217;oxydation, la corrosion, l&#8217;abrasion, les contraintes m\u00e9caniques et la fatigue tout en fonctionnant \u00e0 haute temp\u00e9rature, Welding Alloys a d\u00e9velopp\u00e9 une gamme d&#8217;aciers inoxydables martensitiques sous le nom de famille de produits <a href=\"https:\/\/welding-alloys.zerobox.co.za\/fr\/application\/consommables-de-soudage-de-rechargement\/?yith_wcan=1&#038;family_name=chromecore-2\">CHROMECORE<\/a>. Cette gamme s\u2019applique dans le reste de la coul\u00e9e continue, \u00e0 savoir dans la zone courbe lors du cintrage et du d\u00e9cintrage ou redressement, et dans la zone horizontale lors de l\u2019extraction.<\/p>\n<p><strong>Pourquoi choisir les aciers inoxydables martensitiques ?<\/strong><\/p>\n<p>Les aciers inoxydables martensitiques sont con\u00e7us pour transformer leur microstructure aust\u00e9nitique en martensite lors du refroidissement, offrant une excellente duret\u00e9 et r\u00e9sistance \u00e0 l&#8217;usure. L&#8217;ajout de chrome et de carbone augmente leur r\u00e9sistance \u00e0 la corrosion et leur r\u00e9sistance m\u00e9canique. D&#8217;autres \u00e9l\u00e9ments d&#8217;alliage, tels que le molybd\u00e8ne, le vanadium et\/ou l&#8217;azote, am\u00e9liorent leurs performances \u00e0 haute temp\u00e9rature et contribuent au durcissement.<\/p>\n<p>La gamme CHROMECORE comprend diverses formulations adapt\u00e9es \u00e0 des besoins sp\u00e9cifiques. Voici deux exemples de nos best-sellers :<\/p>\n<ul>\n<li><strong>CHROMECORE 414N :<\/strong> Renforc\u00e9 avec de l&#8217;azote pour am\u00e9liorer les propri\u00e9t\u00e9s m\u00e9caniques et la r\u00e9sistance \u00e0 la corrosion. Ce grade est adapt\u00e9 pour lutter contre les probl\u00e8mes d&#8217;oxydation, mais offre une r\u00e9sistance m\u00e9canique l\u00e9g\u00e8rement inf\u00e9rieure.<\/li>\n<li><strong>CHROMECORE 414MM :<\/strong> Contient du molybd\u00e8ne, du vanadium et du niobium, offrant une excellente duret\u00e9 et r\u00e9sistance \u00e0 l&#8217;usure. Ce grade est id\u00e9al pour les segments d\u2019extraction dans la partie horizontale de la coul\u00e9e, o\u00f9 la r\u00e9sistance m\u00e9canique est cruciale.<\/li>\n<\/ul>\n<p><strong>Innovation:<\/strong><\/p>\n<p>Nous sommes passionn\u00e9s par l&#8217;innovation et nous nous effor\u00e7ons de d\u00e9velopper de nouvelles solutions pour r\u00e9pondre aux exigences de nos clients. Notre nouveau CHROMECORE 414NX am\u00e9liore la durabilit\u00e9 et les performances de l&#8217;ensemble de votre proc\u00e9d\u00e9 de coul\u00e9e continue. Une solution polyvalente unique. Cet acier inoxydable martensitique alli\u00e9 \u00e0 l&#8217;azote et aux \u00e9l\u00e9ments de terres rares offre une r\u00e9sistance exceptionnelle \u00e0 l&#8217;oxydation. Combin\u00e9 au vanadium et au niobium pour un excellent durcissement et une r\u00e9sistance \u00e0 haute temp\u00e9rature, cette innovation maximise les performances de vos rouleaux de coul\u00e9e, et par cons\u00e9quent, celles de votre coul\u00e9e continue dans son int\u00e9gralit\u00e9.<\/p>\n<p>Bien que nous ayons mis en avant quelques produits cl\u00e9s, nous avons une gamme compl\u00e8te de fils fourr\u00e9s, allant des alternatives les plus \u00e9conomiques aux solutions les plus avanc\u00e9es, garantissant un \u00e9quilibre optimal entre durabilit\u00e9 et co\u00fbt pour chaque besoin.<\/p>\n<p><strong>Expertise en fabrication<\/strong><\/p>\n<p>Welding Alloys met \u00e0 profit son expertise approfondie pour produire des fils fourr\u00e9s avec des \u00e9l\u00e9ments d&#8217;alliage soigneusement contr\u00f4l\u00e9s, garantissant l&#8217;obtention de la duret\u00e9 et des propri\u00e9t\u00e9s chimiques souhait\u00e9es. Nous offrons un large choix, permettant aux utilisateurs de s\u00e9lectionner le fil le mieux adapt\u00e9 \u00e0 leur proc\u00e9d\u00e9 de soudage, qu&#8217;il s&#8217;agisse de soudage \u00e0 l&#8217;arc submerg\u00e9 (SAW) ou de soudage \u00e0 l&#8217;arc avec fil fourr\u00e9 auto-prot\u00e9g\u00e9 (FCAW-S).<\/p>\n<p>En plus de nos consommables haute performance CHROMECORE et CORRESIST, Welding Alloys propose une solution compl\u00e8te pour prot\u00e9ger les rouleaux de coul\u00e9e continue, incluant notre automate de soudage fixe, la <a href=\"https:\/\/welding-alloys.zerobox.co.za\/fr\/produit\/automate-de-soudage-profile-roll-cladder\/\">Roll Cladder<\/a>. Cette machine robuste et \u00e0 la pointe de la technologie assure une efficacit\u00e9 et une qualit\u00e9 optimales dans le rechargement, contribuant \u00e0 prolonger la dur\u00e9e de vie des rouleaux et \u00e0 r\u00e9duire leur usure. En combinant technologie innovante et focus sur la qualit\u00e9, nous relevons les d\u00e9fis les plus exigeants en mati\u00e8re d&#8217;usure des rouleaux de coul\u00e9e continue, en offrant des solutions qui r\u00e9pondent aux normes les plus \u00e9lev\u00e9es de l&#8217;industrie sid\u00e9rurgique.<\/p>\n<\/div><\/section><\/div><\/div><!--close column table wrapper. Autoclose: 1 -->\n<style type=\"text\/css\" data-created_by=\"avia_inline_auto\" id=\"style-css-av-av_one_full-a016e44a386b0073341ecd353eaa4e08\">\n.flex_column.av-av_one_full-a016e44a386b0073341ecd353eaa4e08{\npadding:30px 45px 0px 45px;\nbackground-color:#f2f2f2;\n}\n<\/style>\n<div  class='flex_column av-av_one_full-a016e44a386b0073341ecd353eaa4e08 av_one_full  avia-builder-el-9  el_after_av_one_full  avia-builder-el-last  first flex_column_div av-animated-generic right-to-left  column-top-margin'     ><p>\n<style type=\"text\/css\" data-created_by=\"avia_inline_auto\" id=\"style-css-av-m1p1ad97-0b858e81c9e92ca6d185248c4dfb1bf5\">\n#top .av-special-heading.av-m1p1ad97-0b858e81c9e92ca6d185248c4dfb1bf5{\npadding-bottom:10px;\n}\nbody .av-special-heading.av-m1p1ad97-0b858e81c9e92ca6d185248c4dfb1bf5 .av-special-heading-tag .heading-char{\nfont-size:25px;\n}\n.av-special-heading.av-m1p1ad97-0b858e81c9e92ca6d185248c4dfb1bf5 .av-subheading{\nfont-size:15px;\n}\n<\/style>\n<div  class='av-special-heading av-m1p1ad97-0b858e81c9e92ca6d185248c4dfb1bf5 av-special-heading-h3 blockquote modern-quote modern-centered  avia-builder-el-10  el_before_av_gallery  avia-builder-el-first '><h3 class='av-special-heading-tag '  itemprop=\"headline\"  >Galerie<\/h3><div class=\"special-heading-border\"><div class=\"special-heading-inner-border\"><\/div><\/div><\/div><br \/>\n\n<style type=\"text\/css\" data-created_by=\"avia_inline_auto\" id=\"style-css-av-m1hmd14f-242308c40036f6e95a2d3d2f200418a4\">\n#top .avia-gallery.av-m1hmd14f-242308c40036f6e95a2d3d2f200418a4 .avia-gallery-thumb a{\nwidth:100%;\n}\n<\/style>\n<div  class='avia-gallery av-m1hmd14f-242308c40036f6e95a2d3d2f200418a4 avia_animate_when_visible  avia-builder-el-11  el_after_av_heading  avia-builder-el-last  four-col-slider deactivate_avia_lazyload avia-gallery-animate avia-gallery-1'  itemprop=\"image\" itemscope=\"itemscope\" itemtype=\"https:\/\/schema.org\/ImageObject\" ><meta itemprop=\"contentURL\" content=\"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/\"><div class='avia-gallery-thumb'><a href=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine.jpg\" data-srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine.jpg 1000w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-300x231.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-768x592.jpg 768w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-705x544.jpg 705w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-450x347.jpg 450w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-600x463.jpg 600w\" data-sizes=\"(max-width: 1000px) 100vw, 1000px\" data-rel='gallery-1' data-prev-img='https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-300x300.jpg' class='first_thumb lightbox ' data-onclick='1' title=''  itemprop=\"thumbnailUrl\"  ><img decoding=\"async\" fetchpriority=\"high\" class=\"wp-image-51985 avia-img-lazy-loading-not-51985\"  data-avia-tooltip='Recubrimiento de rodillos con alambre tubular CHROMECORE y nuestra m\u00e1quina de soldadura Roll Cladder' src=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-300x300.jpg\" width=\"300\" height=\"300\"  title='Cladding of rolls with CHROMECORE cored wire and our Roll Cladder Machine' alt='Cladding of rolls with CHROMECORE cored wire and our Roll Cladder Machine' srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-300x300.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-80x80.jpg 80w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-36x36.jpg 36w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-180x180.jpg 180w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-120x120.jpg 120w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-450x450.jpg 450w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-100x100.jpg 100w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><div class='big-prev-fake'><img decoding=\"async\" fetchpriority=\"high\" class=\"wp-image-51985 avia-img-lazy-loading-not-51985\"  width=\"300\" height=\"300\" src=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-300x300.jpg\" title='Cladding of rolls with CHROMECORE cored wire and our Roll Cladder Machine' alt='Cladding of rolls with CHROMECORE cored wire and our Roll Cladder Machine' srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-300x300.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-80x80.jpg 80w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-36x36.jpg 36w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-180x180.jpg 180w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-120x120.jpg 120w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-450x450.jpg 450w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-100x100.jpg 100w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/div><\/a><a href=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST.jpg\" data-srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST.jpg 1000w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-300x140.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-768x359.jpg 768w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-705x330.jpg 705w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-450x211.jpg 450w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-600x281.jpg 600w\" data-sizes=\"(max-width: 1000px) 100vw, 1000px\" data-rel='gallery-1' data-prev-img='https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-300x300.jpg' class='first_thumb lightbox ' data-onclick='2' title=''  itemprop=\"thumbnailUrl\"  ><img decoding=\"async\" fetchpriority=\"high\" class=\"wp-image-51981 avia-img-lazy-loading-not-51981\"  data-avia-tooltip='Recubrimiento con CORRESIST' src=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-300x300.jpg\" width=\"300\" height=\"300\"  title='Top roll_ Cladding with CORRESIST' alt='Top roll_ Cladding with CORRESIST' srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-300x300.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-80x80.jpg 80w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-36x36.jpg 36w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-180x180.jpg 180w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-120x120.jpg 120w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-450x450.jpg 450w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-100x100.jpg 100w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><div class='big-prev-fake'><img decoding=\"async\" fetchpriority=\"high\" class=\"wp-image-51981 avia-img-lazy-loading-not-51981\"  width=\"300\" height=\"300\" src=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-300x300.jpg\" title='Top roll_ Cladding with CORRESIST' alt='Top roll_ Cladding with CORRESIST' srcset=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-300x300.jpg 300w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-80x80.jpg 80w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-36x36.jpg 36w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-180x180.jpg 180w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-120x120.jpg 120w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-450x450.jpg 450w, https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Top-roll_-Cladding-with-CORRESIST-100x100.jpg 100w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/div><\/a><\/div><\/div><\/p><\/div><\/div><\/div><\/div><!-- close content main div --><\/div><\/div><div id='after_section_2'  class='main_color av_default_container_wrap container_wrap sidebar_left'  ><div class='container av-section-cont-open' ><div class='template-page content  av-content-small units'><div class='post-entry post-entry-type-page post-entry-52064'><div class='entry-content-wrapper clearfix'><div class='flex_column_table av-av_one_full-9f9a9730a83cca1abdb0fec9b6a55098 sc-av_one_full av-equal-height-column-flextable'><div  class='flex_column av-av_one_full-9f9a9730a83cca1abdb0fec9b6a55098 av_one_full  avia-builder-el-12  el_after_av_section  avia-builder-el-no-sibling  text-center first no_margin flex_column_table_cell av-equal-height-column av-align-top av-animated-generic left-to-right  '     ><p><div  class='avia-button-wrap av-av_button-b69b9cc19ae0d9bfef8ab7b28037331d-wrap avia-button-left  avia-builder-el-13  el_before_av_button  avia-builder-el-first '><a href='https:\/\/welding-alloys.zerobox.co.za\/fr\/societe\/actualites\/'  class='avia-button av-av_button-b69b9cc19ae0d9bfef8ab7b28037331d av-link-btn avia-icon_select-yes-left-icon avia-size-medium avia-position-left avia-color-dark'   aria-label=\"Toutes les actualit\u00e9s\"><span class='avia_button_icon avia_button_icon_left avia-iconfont avia-font-custom' data-av_icon='\ue802' data-av_iconfont='custom' ><\/span><span class='avia_iconbox_title' >Toutes les actualit\u00e9s<\/span><\/a><\/div><br \/>\n<div  class='avia-button-wrap av-av_button-643181888c323bc934d5463d2bf26e09-wrap avia-button-left  avia-builder-el-14  el_after_av_button  avia-builder-el-last '><a href='https:\/\/welding-alloys.zerobox.co.za\/fr\/contactez-nous\/'  class='avia-button av-av_button-643181888c323bc934d5463d2bf26e09 av-link-btn avia-icon_select-yes-right-icon avia-size-medium avia-position-left avia-color-dark'   aria-label=\"Contactez-nous pour en savoir plus\"><span class='avia_iconbox_title' >Contactez-nous pour en savoir plus<\/span><span class='avia_button_icon avia_button_icon_right avia-iconfont avia-font-custom' data-av_icon='\ue803' data-av_iconfont='custom' ><\/span><\/a><\/div><\/p><\/div><\/div><!--close column table wrapper. Autoclose: 1 --><\/p>\n","protected":false},"excerpt":{"rendered":"<p>La coul\u00e9e continue joue un r\u00f4le essentiel dans l&#8217;industrie sid\u00e9rurgique, en transformant l&#8217;acier en fusion en brames, billettes ou blooms.<\/p>\n","protected":false},"author":1,"featured_media":51989,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"_relevanssi_hide_post":"","_relevanssi_hide_content":"","_relevanssi_pin_for_all":"","_relevanssi_pin_keywords":"","_relevanssi_unpin_keywords":"","_relevanssi_related_keywords":"","_relevanssi_related_include_ids":"","_relevanssi_related_exclude_ids":"","_relevanssi_related_no_append":"","_relevanssi_related_not_related":"","_relevanssi_related_posts":"","_relevanssi_noindex_reason":"","inline_featured_image":false,"footnotes":"","_links_to":"","_links_to_target":""},"categories":[11087],"tags":[],"technical-articles-filter":[],"class_list":["post-52064","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-siderurgie"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.7 (Yoast SEO v27.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue | Welding Alloys<\/title>\n<meta name=\"description\" content=\"La coul\u00e9e continue joue un r\u00f4le essentiel dans l&#039;industrie sid\u00e9rurgique, en transformant l&#039;acier en fusion en brames, billettes ou blooms.\" \/>\n<meta name=\"robots\" content=\"noindex, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<meta property=\"og:locale\" content=\"fr_FR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue\" \/>\n<meta property=\"og:description\" content=\"La coul\u00e9e continue joue un r\u00f4le essentiel dans l&#039;industrie sid\u00e9rurgique, en transformant l&#039;acier en fusion en brames, billettes ou blooms.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/\" \/>\n<meta property=\"og:site_name\" content=\"Welding Alloys\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/weldingalloysgroup\" \/>\n<meta property=\"article:published_time\" content=\"2024-09-30T06:10:10+00:00\" \/>\n<meta property=\"article:modified_time\" content=\"2024-09-30T13:20:35+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg\" \/>\n\t<meta property=\"og:image:width\" content=\"400\" \/>\n\t<meta property=\"og:image:height\" content=\"200\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/jpeg\" \/>\n<meta name=\"author\" content=\"thoughtcorp\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\u00c9crit par\" \/>\n\t<meta name=\"twitter:data1\" content=\"thoughtcorp\" \/>\n\t<meta name=\"twitter:label2\" content=\"Dur\u00e9e de lecture estim\u00e9e\" \/>\n\t<meta name=\"twitter:data2\" content=\"5 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/\"},\"author\":{\"name\":\"thoughtcorp\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#\\\/schema\\\/person\\\/d8f86a7cb9a08e431c9ca315ae84574e\"},\"headline\":\"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue\",\"datePublished\":\"2024-09-30T06:10:10+00:00\",\"dateModified\":\"2024-09-30T13:20:35+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/\"},\"wordCount\":3308,\"publisher\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/wp-content\\\/uploads\\\/2024\\\/09\\\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg\",\"articleSection\":[\"Actualit\u00e9s sid\u00e9rurgie\"],\"inLanguage\":\"fr-FR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/\",\"url\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/\",\"name\":\"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue | Welding Alloys\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/wp-content\\\/uploads\\\/2024\\\/09\\\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg\",\"datePublished\":\"2024-09-30T06:10:10+00:00\",\"dateModified\":\"2024-09-30T13:20:35+00:00\",\"description\":\"La coul\u00e9e continue joue un r\u00f4le essentiel dans l'industrie sid\u00e9rurgique, en transformant l'acier en fusion en brames, billettes ou blooms.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#breadcrumb\"},\"inLanguage\":\"fr-FR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"fr-FR\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#primaryimage\",\"url\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/wp-content\\\/uploads\\\/2024\\\/09\\\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg\",\"contentUrl\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/wp-content\\\/uploads\\\/2024\\\/09\\\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg\",\"width\":400,\"height\":200,\"caption\":\"Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/actualites\\\/siderurgie\\\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/accueil\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#website\",\"url\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/\",\"name\":\"Welding Alloys\",\"description\":\"Welding Alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"fr-FR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#organization\",\"name\":\"Welding Alloys\",\"url\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"fr-FR\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/wp-content\\\/uploads\\\/2022\\\/02\\\/logo.png\",\"contentUrl\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/wp-content\\\/uploads\\\/2022\\\/02\\\/logo.png\",\"width\":542,\"height\":279,\"caption\":\"Welding Alloys\"},\"image\":{\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/weldingalloysgroup\",\"https:\\\/\\\/www.youtube.com\\\/user\\\/WeldingAlloystv\",\"https:\\\/\\\/www.instagram.com\\\/weldingalloys\\\/\",\"https:\\\/\\\/linkedin.com\\\/company\\\/welding-alloys\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/welding-alloys.zerobox.co.za\\\/fr\\\/#\\\/schema\\\/person\\\/d8f86a7cb9a08e431c9ca315ae84574e\",\"name\":\"thoughtcorp\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"fr-FR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/4f16b591568093eea1df129490a7e054ccdf41bdb776d3a8b0098f29c8c1ba13?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/4f16b591568093eea1df129490a7e054ccdf41bdb776d3a8b0098f29c8c1ba13?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/4f16b591568093eea1df129490a7e054ccdf41bdb776d3a8b0098f29c8c1ba13?s=96&d=mm&r=g\",\"caption\":\"thoughtcorp\"},\"sameAs\":[\"https:\\\/\\\/www.welding-alloys.com\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue | Welding Alloys","description":"La coul\u00e9e continue joue un r\u00f4le essentiel dans l'industrie sid\u00e9rurgique, en transformant l'acier en fusion en brames, billettes ou blooms.","robots":{"index":"noindex","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"og_locale":"fr_FR","og_type":"article","og_title":"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue","og_description":"La coul\u00e9e continue joue un r\u00f4le essentiel dans l'industrie sid\u00e9rurgique, en transformant l'acier en fusion en brames, billettes ou blooms.","og_url":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/","og_site_name":"Welding Alloys","article_publisher":"https:\/\/www.facebook.com\/weldingalloysgroup","article_published_time":"2024-09-30T06:10:10+00:00","article_modified_time":"2024-09-30T13:20:35+00:00","og_image":[{"width":400,"height":200,"url":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg","type":"image\/jpeg"}],"author":"thoughtcorp","twitter_card":"summary_large_image","twitter_misc":{"\u00c9crit par":"thoughtcorp","Dur\u00e9e de lecture estim\u00e9e":"5 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#article","isPartOf":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/"},"author":{"name":"thoughtcorp","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#\/schema\/person\/d8f86a7cb9a08e431c9ca315ae84574e"},"headline":"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue","datePublished":"2024-09-30T06:10:10+00:00","dateModified":"2024-09-30T13:20:35+00:00","mainEntityOfPage":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/"},"wordCount":3308,"publisher":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#organization"},"image":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#primaryimage"},"thumbnailUrl":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg","articleSection":["Actualit\u00e9s sid\u00e9rurgie"],"inLanguage":"fr-FR"},{"@type":"WebPage","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/","url":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/","name":"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue | Welding Alloys","isPartOf":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#website"},"primaryImageOfPage":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#primaryimage"},"image":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#primaryimage"},"thumbnailUrl":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg","datePublished":"2024-09-30T06:10:10+00:00","dateModified":"2024-09-30T13:20:35+00:00","description":"La coul\u00e9e continue joue un r\u00f4le essentiel dans l'industrie sid\u00e9rurgique, en transformant l'acier en fusion en brames, billettes ou blooms.","breadcrumb":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#breadcrumb"},"inLanguage":"fr-FR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/"]}]},{"@type":"ImageObject","inLanguage":"fr-FR","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#primaryimage","url":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg","contentUrl":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2024\/09\/Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT.jpg","width":400,"height":200,"caption":"Cladding-of-rolls-with-CHROMECORE-cored-wire-and-our-Roll-Cladder-Machine-FEAT"},{"@type":"BreadcrumbList","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/actualites\/siderurgie\/comprendre-et-combattre-lusure-sur-les-rouleaux-de-coulee-continue\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/welding-alloys.zerobox.co.za\/fr\/accueil\/"},{"@type":"ListItem","position":2,"name":"Comprendre et Combattre L\u2019usure sur les Rouleaux de Coul\u00e9e Continue"}]},{"@type":"WebSite","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#website","url":"https:\/\/welding-alloys.zerobox.co.za\/fr\/","name":"Welding Alloys","description":"Welding Alloys","publisher":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/welding-alloys.zerobox.co.za\/fr\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"fr-FR"},{"@type":"Organization","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#organization","name":"Welding Alloys","url":"https:\/\/welding-alloys.zerobox.co.za\/fr\/","logo":{"@type":"ImageObject","inLanguage":"fr-FR","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#\/schema\/logo\/image\/","url":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/02\/logo.png","contentUrl":"https:\/\/welding-alloys.zerobox.co.za\/wp-content\/uploads\/2022\/02\/logo.png","width":542,"height":279,"caption":"Welding Alloys"},"image":{"@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/weldingalloysgroup","https:\/\/www.youtube.com\/user\/WeldingAlloystv","https:\/\/www.instagram.com\/weldingalloys\/","https:\/\/linkedin.com\/company\/welding-alloys"]},{"@type":"Person","@id":"https:\/\/welding-alloys.zerobox.co.za\/fr\/#\/schema\/person\/d8f86a7cb9a08e431c9ca315ae84574e","name":"thoughtcorp","image":{"@type":"ImageObject","inLanguage":"fr-FR","@id":"https:\/\/secure.gravatar.com\/avatar\/4f16b591568093eea1df129490a7e054ccdf41bdb776d3a8b0098f29c8c1ba13?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/4f16b591568093eea1df129490a7e054ccdf41bdb776d3a8b0098f29c8c1ba13?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/4f16b591568093eea1df129490a7e054ccdf41bdb776d3a8b0098f29c8c1ba13?s=96&d=mm&r=g","caption":"thoughtcorp"},"sameAs":["https:\/\/www.welding-alloys.com"]}]}},"_links":{"self":[{"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/posts\/52064","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/comments?post=52064"}],"version-history":[{"count":2,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/posts\/52064\/revisions"}],"predecessor-version":[{"id":52066,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/posts\/52064\/revisions\/52066"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/media\/51989"}],"wp:attachment":[{"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/media?parent=52064"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/categories?post=52064"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/tags?post=52064"},{"taxonomy":"technical-articles-filter","embeddable":true,"href":"https:\/\/welding-alloys.zerobox.co.za\/fr\/wp-json\/wp\/v2\/technical-articles-filter?post=52064"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}